All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
new zealand halloysite 25.00
minspar 200 feldspar 23.00
super standard porcelain 27.00
silica 25.00
Add Amount
veegum t 2.00

Instructions

Super Standard porcelain is a very white kaolin. This clay body (S.W.F.T. or Super White Fairly Translucent) is most plastic and workable when mixed as a slip and dried out on plaster. It shrinks about 18%. I fire on alumina wash rather than kiln wash as it will take on the uneven texture.
To make colored clays, I add 2–8% ceramic stains. 

This recipe was shared by Chris Alveshere in the January/February 2022 issue of Pottery Making Illustrated.