All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 20.60
Custer Feldspar 28.90
EPK Kaolin 18.90
silica 31.60
Add Amount
Rutile 7.00

Instructions

To get the rivulets shown here, apply Red- Black Glaze and Mel’s Orange Underglaze, then layer over the top half of the piece with any rutile base from Glazy.org, such as the recipe shown above. 

 

This recipe was shared by Mark Cortright in the October 2021 issue of Ceramics Monthly.