All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 6.00
Wollastonite 15.00
ferro frit 3124 20.00
Custer Feldspar 20.00
EPK Kaolin 20.00
silica 19.00
Add Amount
gold-chloride 0.04

Instructions

To achieve good color results, thicker application is better, as this glaze is incredibly stable and does not run much. If firing in oxidation, a medium firing ramp with a 15-minute hold at the top temperature is sufficient to let any off-gassing pinholes seal over. 

 

The tile on the left was fired to cone 6 in oxidation. The tile on the right was fired to cone 10 in reduction.

 

This recipe was shared by Ryan Coppage in the October 2021 issue of Ceramics Monthly.