All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldpsar 51.00
Gerstley Borate 21.00
Whiting 7.00
OM 4 Ball Clay 2.00
Silica 19.00
Add Amount
Copper Carbonate 2.00

Instructions

Viva Clayworks studio in Edmonton, Alberta, has been using this recipe for 28 years. The origins have been lost, but the beauty of it stands as a testament to the inventor.

This recipe was shared by Kirsty Kash in the May/June 2023 issue of Pottery Making Illustrated.