All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 16.00
Potash Feldspar 56.00
EPK Kaolin 7.00
silica-(325-mesh) 21.00
Add Amount
Red Iron Oxide 10.00

Instructions

Only a quick dip is needed to apply this glaze as it will run if applied too thick. Fire this glaze to cone 10 in reduction in a gas kiln. 

 

This recipe was shared by Mark Cortright in the October 2021 issue of Ceramics Monthly.