All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 30.00
EPK Kaolin 10.00
Grolleg Porcelain 50.00
Newman Red Clay 10.00

Instructions

This extremely reliable slip does well in both wood and soda firings. Mix to skim milk consistency, then apply to bisque-fired work. Yields dark oranges, browns, reds, and black.

 

This recipe was shared by Johnny Arvizu in the February 2024 issue of Ceramics Monthly.