All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
gerstley borate 50.00
plastic vitrox clay 50.00

Instructions

Mix to a slightly thick consistency (like heavy cream) and apply to bisqueware via dipping, pouring, or spraying. 

 

This glaze is fired in a train-style wood kiln using mixed hardwoods. Firing duration and temperature: 27-hour firing to cone 10–11, cooled in reduction for roughly 6 hours (stoking
4 small to medium sticks of side-stoke wood in the primary air and side-stoke ports about every 15 minutes until the temperature reached 1500°F (816°C) in the front of the kiln and 1600°F (871°C) in the back of the kiln). 

 

This recipe was shared by Seth Green in the December 2021 issue of Ceramics Monthly.