All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 6.40
Gerstley Borate 12.70
Talc 13.60
Minspar 200 37.40
EPK Kaolin 4.50
Silica 22.70
Zinc Oxide 2.70
Add Amount
Cobalt Oxide 2.00
Bentonite 2.00

Instructions

Combines in interesting ways with other glazes, where it encourages additional crystal growth. 

For the three or more glaze combination tests, I dipped the entire piece in the first glaze for two seconds, let it dry, then inverted the piece and dipped a second glaze for one second. The pieces were then allowed to dry, at which point a third glaze was applied by inverting the pieces and glazing the top one-quarter for one second. The image shown with this recipe shows Sunshine + Spearmint + Pike's Purple.

This recipe was shared in the January 2025 issue of Ceramics Monthly as an excerpt from Odyssey ClayWorks Director Gabriel Kline’s Amazing Glaze Recipes and Combinations, published by Quarto Press.