All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 30.00
Grolleg Kaolin 65.00
Silica 5.00
Add Amount
Bentonite 1.00
Titanium Dioxide 5.00

Instructions

Mix this slip to the consistency of half and half. It can be brushed or dipped. In oxidation firings, this slip tends to lean into a soft, butter yellow. In heavy reduction, however, it will fire to a toasty orange. It can be very resistant to atmospheric effects, so it usually comes out with a matte finish. 

This recipe was shared by Eric Ordway in the December 2025 issue of Ceramics Monthly.