All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wood Ash 40.00
Custer Feldspar 33.00
Silica 27.00
Add Amount
borax 5.00

Instructions

With this glaze, I usually double dip pieces, which means the surface can be very delicate and prone to flaking off if not gently handled. In the firing, the glaze has a tendency to run significantly when it gets to temperature, so I recommend making a wadding disk or cookie to fire the piece on to help minimize the damage to shelves. I recommend mixing to a heavy-whipping-cream consistency and dipping to apply. 

This recipe was shared by Eric Ordway in the December 2025 issue of Ceramics Monthly.