All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 29.00
Ferro Frit 3195 20.00
Nepheline Syenite 4.00
EPK Kaolin 30.00
Silica 17.00
Add Amount
Dark Rutile 6.00
Manganese Dioxide 4.00

Instructions

Oatmeal is a versatile glaze that has a reduction look. Oatmeal suggests fall colors and forms a wonderful two-glaze combination with Campana Grey. 

This recipe was shared in the January 2025 issue of Ceramics Monthly as an excerpt from Odyssey ClayWorks Director Gabriel Kline’s Amazing Glaze Recipes and Combinations, published by Quarto Press.