All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 30.00
Ferro Frit 3124 15.00
Ball Clay 40.00
Calcined Kaolin 15.00
Add Amount
Zircopax 5.00

Instructions

This was a Nova Scotia College of Art and Design (NSCAD) shop slip. For application on leather-hard clay, it can be brushed, dipped, and poured. Do not use on bisqueware. I fire to cone 04 for bisque and cone 05 for the glaze firing.

This recipe was shared by Lindsay Montgomery in the November 2025 issue of Ceramics Monthly.