All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 6.00
EPK Kaolin 47.00
OM 4 Ball Clay 47.00
Add Amount
Zircopax 12.00
Bentonite 2.00
Titanium Dioxide 7.00

Instructions

I was looking for a new orange flashing slip when I stumbled upon this combination. I would say that this one has an electric quality to the yellow that interacts more favorably than my old yellow flashing slip has. Mix to a half-and-half consistency. It can be brushed or dipped.

This recipe was shared by Eric Ordway in the December 2025 issue of Ceramics Monthly.