All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 30.00
EPK Kaolin 10.00
Grolleg 50.00
Newman Red Clay 10.00
Add Amount
Bentonite 3.00

Instructions

Mix to a water-thin consistency for dipping or spraying.

This recipe was shared by Ben Eberle in the December 2025 issue of Ceramics Monthly.