All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
minspar 21.95
OM 4 Ball Clay 30.49
tennessee-9-ball-clay 17.07
Tile 6 30.49
Add Amount
mullite-200-mesh 6.02
pyrax-hs 16.87

Instructions

This is my newest clay body that has been pretty great so far after switching from B-Mix earlier this year. It’s a Casey Beck body that I’ve modified.