All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 22.10
Custer Feldspar 60.12
EPK Kaolin 17.78
Add Amount
Zinc Oxide 6.50
Red Iron Oxide 5.40
Rutile 10.92

Instructions

This is a runny underglaze. I fire it to cone 10 in reduction in a gas kiln. 

This recipe was shared by Mark Cortright in the October 2021 issue of Ceramics Monthly.