All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
strontium carbonate 3.09
whiting 17.68
minspar 200 feldspar 44.13
nepheline syenite 26.45
epk kaolin 8.65
Add Amount
titanium dioxide 6.18
zinc oxide 8.78
rutile 6.18

Instructions

Mix to a skim-milk consistency. Works well when layered under the Crystal Clear glaze. When layering, make sure to stir continuously, as the rutile will settle. 

 

This recipe was shared by Abby Reczek in the February 2022 issue of Ceramics Monthly.