All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 43.00
Ferro Frit 3195 43.00
EPK Kaolin 14.00

Instructions

I use this glaze and the satin base glaze similarly, brushing, dipping, or pouring as needed. I use it thick or thin, depending on the effect I’m looking for. If it gets too thin it will come out dry.

 

This recipe was shared by Maggie Jaszczak in the March 2024 issue of Ceramics Monthly.