All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 65.80
Minspar 200 Feldspar 17.20
Nepheline Syenite 6.20
EPK Kaolin 10.80
Add Amount
Tin Oxide 4.00
Zircopax 9.00
Bentonite 2.00
Mason Stain 6242 Bermuda Green 2.00

Instructions

I add 2% Mason stain 6242 Bermuda green. I mix a 2-gallon bucket (5000 g) of this glaze and add 1 teaspoon of Epsom salts to the batch.

This recipe was shared by Sam Momeyer in the November/December 2023 issue of Pottery Making Illustrated.