All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
ferro frit 3124 65.80
minspar 200 feldspar 17.20
nepheline syenite 6.20
EPK Kaolin 10.80
Add Amount
tin-oxide 4.00
zircopax 9.00
BENTONITE 2.00

Instructions

I add anywhere from 1–5% of various Mason stains (MS) to the glaze base to achieve a wide range
of colors. To prevent settling, add 1–3 teaspoons Epsom salts per 5000-gram batch size. 

 

This recipe was shared by Mark Arnold in the September 2022 issue of Ceramics Monthly.