All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
laterite 100.00

Instructions

To create this slip, use as much laterite as needed to make an appropriate-sized batch and add enough water to create a thin slip. Apply this to bisqueware via dipping, pouring, spraying, or brushing. Works best in wood firings. 

 

This slip is fired in a train-style wood kiln using mixed hardwoods. Firing duration and temperature: 27-hour firing to cone 10–11, cooled in reduction for roughly 6 hours (stoking
4 small to medium sticks of side-stoke wood in the primary air and side-stoke ports about every 15 minutes until the temperature reached 1500°F (816°C) in the front of the kiln and 1600°F (871°C) in the back of the kiln). 

 

This recipe was shared by Seth Green in the December 2021 issue of Ceramics Monthly.