All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 4.03
Dolomite 8.06
Gerstley Borate 8.06
Whiting 2.42
ZInc Oxide 12.89
Potash Feldspar 38.68
EPK Kaolin 1.69
silica-(325-mesh) 24.17
Add Amount
Copper Carbonate 1.77
tin-oxide 2.42

Instructions

This glaze is fired to cone 10 in reduction in a gas kiln. Apply glaze just a bit thicker than usual glazing. Start reduction at 1750°F (954°C). 

 

 This recipe was shared by Mark Cortright in the October 2021 issue of Ceramics Monthly.