All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3134 50.00
EPK Kaolin 30.00
Silica 20.00
Add Amount
Bentonite 2.00
Zircopax 12.50
Lithium Carbonate 1.00

Instructions

For this glaze, I altered the original recipe slightly by decreasing the Zircopax and adding a little lithium carbonate. This makes the glaze break over texture nicely and slightly shinier. This glaze looks best when slow cooled. I adapted this recipe, with a couple of adjustments, from John Britt’s book The Complete Guide to Mid-Range Glazes. 

This recipe was shared by Kyla Strid in the January 2025 issue of Ceramics Monthly.