All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 18.00
Strontium Carbonate 2.00
Whiting 8.00
Custer Feldpsar 54.00
EPK Kaolin 5.00
Silica 9.00
Zinc Oxide 4.00
Add Amount
Light Rutile 3.00
Bentonite 2.50
Cobalt Oxide 2.00
Zircopax 2.00
Titanium Dioxide 2.00

Instructions

A smooth blue that breaks over texture. Works well as a modifier glaze over other glazes. 

For the three or more glaze combination tests, I dipped the entire piece in the first glaze for two seconds, let it dry, then inverted the piece and dipped a second glaze for one second. The pieces were then allowed to dry, at which point a third glaze was applied by inverting the pieces and glazing the top one-quarter for one second. The image shown with this recipe shows Silky Black + Isa's Bomb Blue + Odyssey White Gloss.

This recipe was shared in the January 2025 issue of Ceramics Monthly as an excerpt from Odyssey ClayWorks Director Gabriel Kline’s Amazing Glaze Recipes and Combinations, published by Quarto Press.