All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3134 2.00
Ferro frit 3195 0.50
OM 4 Ball Clay 2.00
Mason stain 1.00
Add Amount
BENTONITE 1.00
gum-solution 1.00

Instructions

Note: Mason Stain and Gum Solution are listed in teaspoons. All other ingredients are listed in tablespoons.

Start with 1 tsp of darker Mason stains and 2 tsp for light Mason stains. Increase the amount as needed. Combine ingredients and run through a 60-mesh sieve. 

 

This recipe was shared by Kimberly Hilligoss in the July/August 2022 issue of Pottery Making Illustrated.