All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Calcium Carbonate 30.00
Strontium Carbonate 10.00
Cedar Heights Red Art 60.00
Iron Oxide 3.50
Yellow Ochre 4.00
Add Amount
iron oxide 3.50
yellow ochre 4.00

Instructions


I apply this glaze to pieces first by painting or trailing (generous coating), then follow with pouring and dipping the piece in Spodumene Glaze.

This recipe was shared by Terry Plasket in the June/July/August 2021 issue of Ceramics Monthly.