All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 4.60
Dolomite 8.30
Whiting 20.40
Ferro Frit 3124 4.60
Minspar 200 48.40
EPK Kaolin 13.70
Add Amount
Titanium Dioxide 13.70
Bentonite 2.30

Instructions

This glaze was shared by Mike Stumbras. It’s white with crystalline variations, and heavy soda creates blue and purple. It pairs well on top of glazes—it is particularly lovely over Tenmoku and porcelain shino. I recommend firing between cones 10 and 11. It will run at hotter temps and be lackluster at cooler temps.

 

This recipe was shared by Samuel Newman in the December 2024 issue of Ceramics Monthly.