All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 10.00
Lithium Carbonate 10.00
Minspar 200 40.00
6 Tile Kaolin 40.00
Add Amount
Rutile 10.00

Instructions

Soda interaction creates gorgeous blues and greens. It fire to a less desirable yellow mustard when too thick or when it has limited soda interaction. Apply in a thin milky consistency. Fire between cones 9 and 11.

 

This recipe was shared by Samuel Newman in the December 2024 issue of Ceramics Monthly.