All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 4.76
Cornwall Stone 11.90
Nepheline Syenite 11.90
Tile 6 23.81
XX Saggar 23.81
Silica 23.81
Add Amount
Zircopax 9.52

Instructions

This recipe is semi-translucent when fired under a glaze. Increase the percentage of Zircopax to make it more opaque.

 

This recipe was shared by Mike Cerv in the March/April 2024 issue of Pottery Making Illustrated.