All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
SODA ASH 18.37
Nepheline Syenite 42.86
Kona F4 Feldspar 10.20
Cedar Heights RedArt 5.10
EPK Kaolin 9.18
Ball Clay 14.29

Instructions

I bisque to cone 012, so I thin my glaze down and apply it quickly. I only use this glaze on black clay in long wood firings. It is interesting on porcelain and gray stoneware but the color is much brighter. Usually this glaze comes out orange. When it is fired for a longer amount of time on a darker clay body it develops gold and copper tones. 

 

This recipe was shared by Will Talbot in the May 2024 issue of Ceramics Monthly.