All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 20.00
Whiting 3.00
nepheline syenite 40.00
EPK Kaolin 13.00
silica 24.00
Add Amount
cobalt carbonate 0.25
Red Iron Oxide 1.00

Instructions

This glaze does not have any special mixing requirements, but if it’s made or applied too thick, it can be runny. 

 

This recipe was shared by Matthew Eames in the October 2022 issue of Ceramics Monthly.