All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley borate 36.00
Spodumene 45.00
silica 19.00

Instructions

I fire this glaze primarily to cone 3 in the soda kiln. 

 

This recipe was shared by Justin Rothshank in the June/July/August 2022 issue of Ceramics Monthly.