All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
dolomite 13.00
lithium carbonate 3.00
whiting 7.00
nepheline syenite 47.00
epk kaolin 2.00
silica 28.00
Add Amount
bentonite 4.00

Instructions

Mix to a skim-milk consistency. Works well when layered over top of the Matte Rutile Glaze. When layering, make sure the Matte Rutile Glaze has fully dried first. 

This recipe was shared by Abby Reczek in the February 2022 issue of Ceramics Monthly.