All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 10.00
Nepheline Syenite 20.00
spg-or-xx-sagger-ball-clay 70.00
Add Amount
Cedar Heights Redart 2.00

Instructions

These slips require ball milling or screening through a 100-mesh sieve. Shown on the bottles above, these slips do well fired to cone 2 in a soda kiln. Recipes shared by Tom Jaszczak in Justin Rothshank’s book, Low-Fire Soda, published by The American Ceramic Society and available at mycan.ceramicartsnetwork.org/s/shop.

This recipe was shared by Tom Jaszczack in the October 2023 issue of Ceramics Monthly.