All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 10.00
Nepheline Syenite 20.00
XX Saggar Ball Clay 70.00

Instructions

I run this slip through the ball mill, and add Mason stains (MS) to it for other color options. I apply most slip leather hard. This slip also looks nice with clear over it in an oxidation firing. 

For black slip, add 4% MS 6650. For gray slip, add 9% of a blend of MS 6650 and MS 6700. For blue slip, add 4–9% of any blue stain.

 

This recipe was shared by Tom Jaszczak in the March 2024 issue of Ceramics Monthly.