All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
whiting 18.56
calcium borate frit 3.09
cornish stone 75.26
zinc oxide 3.09
Add Amount
bentonite 3.09

Instructions

This clear, stoneware-temperature glaze fires to 2336°F (1280°C). The recipe comes from the Guldagergaard International Ceramic Research Center in Skælskør, Denmark. I apply this clear glaze by spraying to a thickness of approximately 1 mm over cobalt oxide, which I purchased in Jingdezhen, China, while traveling.  

 

This recipe was shared by Janina Myronova in the November 2021 issue of Ceramics Monthly.