All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 20.00
ferro frit 3124 25.00
nepheline syenite 25.00
EPK Kaolin 15.00
silica 15.00
Add Amount
BENTONITE 2.00
zircopax 10.00

Instructions

For the bentonite, weigh it in a separate container and dry mix with the other ingredients prior to adding water.

I run the glaze through an 80-mesh sieve.

Depending on the intended look, I will dip or spray this glaze. Currently 90% of my worked is dipped with a 2-second hold in the glaze bucket.

I wax the bottom of all pieces prior to glazing. 

 

This recipe was shared by Rich Brown in the June/July/August 2022 issue of Ceramics Monthly.