All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 20.00
Spodumene 11.00
Ferro Frit 3134 21.00
EPK Kaolin 20.00
Silica 20.00
ZInc Oxide 8.00
Add Amount
Manganese Carbonate 1.80
Copper Carbonate 0.60
Cobalt Carbonate 0.15

Instructions

This gorgeous, fluid, gray/blue glaze breaks beautifully over texture and pools in low-lying areas. Campana Grey works well over the top of other glazes, but can be very runny, so put cookies under these pots. 

 

This recipe was shared in the January 2025 issue of Ceramics Monthly as an excerpt from Odyssey ClayWorks Director Gabriel Kline’s Amazing Glaze Recipes and Combinations, published by Quarto Press.