All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 21.74
Ferro Frit 3134 22.83
Spodumene 11.96
EPK Kaolin 21.73
Silica 325 21.74
Add Amount
Zinc 8.70
sage-mason-stain 5.00
red-brown-mason-stain 3.00
Copper Carbonate 5.00

Instructions

This recipe is used for a liner and then an exterior layer. I use the variations as dots of color over the base glaze layer.  

This recipe was shared by Ray Brown in the September 2024 issue of Ceramics Monthly.