All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 4.63
Ferro Frit 3124 9.26
Nepheline Syenite 24.07
EPK Kaolin 15.74
OM 4 Ball Clay 23.15
Silica 23.15
Add Amount
Titanium Dioxide 9.26
Bentonite 1.85

Instructions


Mix to skim milk consistency. Apply a very thin coat to bisque-fired ware to prevent adhesion issues. The fired color range is yellow to reddish brown.

This recipe was shared by Lisa York in the April 2020 issue of Ceramics Monthly.