All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
wollastonite 24.10
nepheline syenite 27.69
epk kaolin 21.03
silica 27.18
Add Amount
zinc oxide 2.00
bentonite 1.00
red stain 10.00

Instructions

Mix this glaze to the consistency of heavy cream. Apply thickly as accents via brushing. For Pink, combine already mixed batches of White and Red glazes by eye and test to refine results. For all colored stains, I use various Mason stains. 

These recipes are shown applied over a dark clay body. I work mainly with a clay body from STAR- works called DarkSTAR 10, and I also use other high-fire clays from various clay companies.

 This recipe was shared by Minsoo Yuh in the January 2022 issue of Ceramics Monthly.