All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldpsar 10.00
Nepheline Syenite 10.00
EPK Kaolin 15.00
Tile 6 42.00
XX Saggar 5.00
Pyrophyllite 10.00
Silica 8.00
Add Amount
alumina 2.00
bentonite 1.00
molochite 5.00
grog 5.00

Instructions

Fired color ranges of yellows, oranges, browns, and reds. A majority of my work is made with this clay body, and I often pair it with flashing slips.

 

This recipe was shared by Johnny Arvizu in the February 2024 issue of Ceramics Monthly.