All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 20.45
Grolleg Kaolin 28.41
OM4 Ball Clay 28.41
Silica 22.73
Add Amount
Zircopax 5.68

Instructions

This is a super versatile standard white slip. Great thick and thin. Virginia Torrence loves a thin, clear glaze wash over it at cone 6.

For Black: Add: 6600 Mason Stain 8.00 %

This recipe was shared by Virginia Torrence in the April 2024 issue of Ceramics Monthly.