All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 50.00
Nepheline Syenite 16.67
Alumina Hydrate 33.33

Instructions

To achieve a textured green gray like the surface on the rhino, I use a combination of this stain recipe and commercial underglazes and glazes. To create this surface, apply these layers in order: Dark Gray Amaco underglaze, Adrian Arleo's Dark Blue Sand Dry Stain wash, Laguna MS-35 Sage glaze, Laguna MS-46 Agate glaze.

The 5-segment slow-cooling firing schedule I use for my glazes is as follows:

Segment 1: 150°F per hour up to 1200°F.

Segment 2: 200°F per hour up to 2000°F.

Segment 3: 150°F per hour up to 2150°F, with a 15 minute hold at top temperature.

Segment 4: cooling 500°F per hour down to 2000°F, with a 15 minute hold.

Segment 5: Cooling 125°F per hour down to 1400°F. Then the kiln is allowed to cool on its own to ambient temperature.

This recipe was shared by Ariel Bowman in the May 2019 issue of Ceramics Monthly.