All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 6.40
Whiting 13.70
Ferro Frit 3124 27.20
EPK Kaolin 21.00
Silica 31.70

Instructions

The vessel in the image shown here was sprayed with Glendale Community College Gloss first and then Zinc-Free Clear was sprayed over it to add more depth.

Published in "Pour It On! Recipes" by Carly Van Anglen and David Ferro, Alina Hayes, and Justin Donofrio in the September 2017 issue of Ceramics Monthly.
This is a clear glaze I spray on top of the colored Glendale Community College Gloss glaze, to give the surface a bit more depth. The glaze recipe is also from the college.