All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Soda Ash 7.80
Nepheline Syenite 14.60
Soda Feldspar (Minspar 200) 34.00
Spodumene 29.00
EPK Kaolin 9.70
OM 4 Ball Clay 4.90

Instructions


I apply this shino by dipping pieces into the glaze. Original recipe attributed to Zach Tate.

This cup was first dipped in Original Burke Orange. Next, the entire pot was dipped in Zach's Shino. After applying the shino and while the glaze on the surface was still wet, Ferro Frit 3134 was shaken onto the exterior. This pieces was fired to cone 9 in reduction in a gas kiln.

This recipe was shared by Dick Lehman in the the November 2019 issue of Ceramics Monthly.