All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 15.12
Gerstley Borate 6.98
Lithium Carbonate 4.65
Whiting 16.28
Zinc Oxide 0.58
Custer Feldspar 43.02
EPK 13.37
Add Amount
Titanium Dioxide 16.28

Instructions

Published in "Tom and Elaine Coleman" by John Nance, in the Jan 2003 issue of Ceramics Monthly.
This image shows Yellow Crystal Matt and Black Barium Matt Glazes with dry mesquite ash sprinkled on top.

For use on exterior or decorative surfaces. Yields a beautiful butter-smooth glaze that develops crystals. For a yellow-gold, add 2% yellow iron oxide. Responsive to oxide oversprays. For a pumpkin orange, spray with Spotted Black Glaze.