All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 25.03
Dolomite 18.02
Custer Feldspar 16.69
Nepheline Syenite 25.03
EPK Kaolin 9.67
Silica 5.56
Add Amount
Zircopax 6.67
Red Iron Oxide 4.17
Bentonite 0.69

Instructions

Published in "Atmospheric Recipes," in the October 2018 issue of Ceramics Monthly. This recipe has been contributed by Stephen Heywood.
This glaze is not food safe. A thick application works best.