All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 17.90
Ferro Frit 3124 25.80
Nepheline Syenite 14.80
EPK Kaolin 12.20
Silica 29.30
Add Amount
Stain 10.00

Instructions

Originally published in the May 2018 issue of Ceramics Monthly.
This is a sculptural glaze that I fire multiple times to cone 01,03, 04 and 06.