All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 55.00
EPK Kaolin 30.00
Silica 15.00
Add Amount
Degussa Orange Stain 10.00

Instructions

Published in "Working Potter Glazes" in the June 2015 issue of Ceramics Monthly.

Low-fire glossy clear glaze. Holds colorants well, especially for reds and oranges. Try 10% Degussa Orange stain for orange.
Mix all ingredients together prior to adding the water.